Hello TechNet:
We performed some experiments on Immersion White Tin boards and found the
following . . . . First, we had no problems with solder paste application.
Second, no problems with vision systems, etc., and part placement. Third,
solder joints looked pretty good . . i.e. . no problems. Here is the
kicker. The mounting holes on the top side were white tin. The mounting
holes need to be very flat for good contact so we do not apply solder paste
to these holes. The white tin, after exposure to humidity of the
environmental chambers looked very oxidized and a flaky white powdery like
substance was observed. Also under some RF type connectors, the white
powdery like substance was observed. The powdery like flaky substance did
not show up under any other components only the gold RF connectors.
What experience have any of you had with the immersion white tin process?
Any ideas, thoughts, etc., on the powdery white substance??? We are going to
have our "product assurance forensic lab" analyze it and see what they come
up with, but we also thought it a good idea to tap the intelligence of the
TechNet World as well.
Ron Hollandsworth
ITT
************************************
If this email is not intended for you, or you are not responsible for the
delivery of this message to the addressee, please note that this message may
contain ITT Privileged/Proprietary Information. In such a case, you may not
copy or deliver this message to anyone. You should destroy this message and
kindly notify the sender by reply email. Information contained in this
message that does not relate to the business of ITT is neither endorsed by
nor attributable to ITT.
************************************
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|