TECHNET Archives

February 2009

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Kevin Glidden <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Kevin Glidden <[log in to unmask]>
Date:
Wed, 11 Feb 2009 13:59:53 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (133 lines)
Your welcome.  The strings get worse as the pot life window closes.  Mix
small batches and move fast!  It cleans up when wet with IPA & Q-tips pretty
well. 


Kevin Glidden
Manufacturing Engineer
Luminescent Systems Inc.

-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]] 
Sent: Wednesday, February 11, 2009 1:53 PM
To: Kevin Glidden; TechNet E-Mail Forum
Subject: RE: [TN] Staking Question/Help...

Hi Kevin!

Just wanted to let you know that the material we have is exactly the same
material. I said Bergdahl earlier, but that was the distributor.
The stuff that we have IS from PRC-Desoto...

I really appreciate the tips you gave me. I think we can live with a couple
of days to cure instead of a week or more.

I mixed a little up to play around and see for myself how it behaves.
One thing about this stuff is that you can make a real mess if you're not
careful! It "strings" quite a bit when you are applying it.

Thanks again,

Steve

-----Original Message-----
From: Kevin Glidden [mailto:[log in to unmask]]
Sent: Wednesday, February 11, 2009 8:56 AM
To: 'TechNet E-Mail Forum'; Steve Gregory
Subject: RE: [TN] Staking Question/Help...

Hi Steve,

Glad to hear you made it through the storms OK.

I used to use this material extensively, and as luck would have it I was
able to locate some old notes...

The specific material I used was PRC Desoto 1440B.  I am not sure if the PRC
material is different, or if there was some sort of acquisition or merger,
BUT the PRC Desoto sheet called for a 36 hour room temp cure to 35A
durometer in 48 hours, but all the performance data was performed on cured
14 days.

Anyway, I like you, could not tolerate that, so I called the PRC Desoto
technical assistance, and wrote down there response:
------------
Heat Cure can be used.  Must room cure at 1 hr minimum before oven curing to
allow chemical evaporation.  Then place in a 140F to 150F oven for 24 hours.
Failure to observe the one hour at room temperature prior to oven cure will
result in blistering of material.
------------

I never had any issues with this method.  We too used it for bonding of
components, on military backplanes.  In my experience, all 3 major primary
defense contractors use it, and it is prefferred as it has high chemical
resistance, maintains elasticity, and decent dielectric values as well.

One last note is that there is also a B 1/2 formulation available per the
same MIL-spec with a shorter 30 hour RT cure time, but also a shorter pot
life.

Good Luck.

Kevin Glidden
Manufacturing Engineer
Luminescent Systems Inc.


-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: Wednesday, February 11, 2009 9:34 AM
To: [log in to unmask]
Subject: [TN] Staking Question/Help...

Morning All!
 
Well, survived all the storms we had last night. Actually, it wasn't bad in
Tulsa as it was to the south and to the west of us.
 
They think there was a tornado that touched down in a city called Pawnee to
the west, one in Edmond to the south, and there were eight lives lost in
Lone Grove last night. Really early for tornado season here...
 
Anyways, we're building a board that has a requirement to stake some PTH
radial parts and they reference MIL-S-8802, Class B2 as the material to be
used for the staking. Our buyers purchased a 2-part material from Bergdahl
called PR-1440 Class B. So I got the datasheet and started looking at how to
use it, and discovered that the fastest that I can cure it is 7-days at 250
F., or 14-days at room temperature. That really puts a kink in our
schedule... 
 
I'm not very familiar with that spec, but what I can find is that most
everything I find that is listed and complies with it, is actually aircraft
fuel tank sealant. Why they want to use that is beyond me, but that's what
is on the drawing so that what we'll use. 
 
I'm wondering if any of you know of anything that will cure quicker than
that and complies with the above spec? Any help is appreciated.
 
Steve
 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please visit
IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2