Hi Doug,
See my responses below:
>>Steve,
>>I have not used that specific material before, but have worked with 2-part
>>systems. A few questions and observations:
>>1. What did you mix the material with? Metal spatula (good) or popscicle
>>stick (bad)?
Answer: I mixed it with a plastic spatula
>>2. How well did you scrape the sides of the container? Was it a clean
>>plastic mixing cup (good) or wax-coated Dixie cup (bad)?
Answer: I thought I scraped the sides pretty good. It was a clean plastic mixing cup, just a regular kitchen mixing cup with graduations on the sides.
>>3. Did you bake out the potted assemblies first?
Answer: No I did not. In retrospect I should have...
>>4. Was there a primer involved?
Answer: No primer.
>>5. What kinds of "schmutz" may be on the assembly that may poison the
>>cure reaction? Urethanes don't like water.
Answer: I thought the boards were clean. I learned afterwards that there was some no-clean rework done to a programmed part (it was removed and replaced), although I didn't see any residues.
>>6. Does the manufacturer recommend a rest time before potting? Degassing
>>before potting?
Answer: I didn't see any rest time or degassing recommendations in the datasheet.
>>You might want to pick up IPC-HDBK-850, The Potting and Encapsulation
>>Handbook for lots of good information.
Yep, will ask that we get the Handbook.
I called Epic and talked to them about what happened, and they told me that I should mix by weight to be more accurate. So as a test of the material, I did that. I mixed 300-grams of part A to 129-grams of part B (100:43 ratio per the datasheet). Mixed it the same way I did last week, then poured the material into two containers. This time I did the alternate oven cure of 65 C. for 1 to 1.5 hours. It turned out beautiful. Smooth, with no bubbles except for some very tiny ones around the edges of the container. I am at a loss as to why I had the results that I did last week. So frustrating...
Steve
From: stephen gregory <[log in to unmask]>
To: <[log in to unmask]>
Date: 07/22/2013 01:46 PM
Subject: [TN] Epic Resins S7144A 2-part polyurethane potting
material
Sent by: TechNet <[log in to unmask]>
Hi All,
Have any of you used Epic Resins S7144A 2-part polyurethane potting
material?
I tried to last week, and pretty much made a mess. Followed the datasheet
and mixed it in the volume ratio of 3-parts part-A (300-cc) to 1-part
part-B (100-cc). I mixed more material than I actually needed. I'm mixing
it by hand because we don't have a MMD system.
I thought I had mixed everything thoroughly (4-5 minutes). I determined
ahead of time how much material would be needed for each unit (35-cc's).
After mixing, I drew the material into a 60-cc syringe and
dispensed 35-cc into each case. I let it room cure (24-30 hours).
I did 4-units and each one of them had a different result, from swelling
and bubbling of the material completely out of the case, to little or no
cure. I'm at a loss as to why that happened.
Just wondering if any of you have ever used the material and can give me
some pointers.
Thanks guys,
Steve
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|