>Kirk VanDreel
>05/19/97 11:25 AM
>Does any one have the capability to produce 50 um lines and spaces with 2
>um fused solder over the traces?  Experiments have shown a dewetting of the
>solder into balls on the traces, however, the wetting angle is not bad.  Is
>there a physical constraint we are running into which is causing this
>globbing of the solder?
>
Hello Kirk,

I have seen this problem on fine traces caused by excess tin-lead rather
than dewetting. When you etch, the undercut reduces the copper trace
width under the tin-lead. A 50um trace reduced to 40um will effectively
give 20% more tin-lead thickness when fusing, and above a certain
thickness it will bunch up due to surface tension and produce a solder
ball. Having said that, I would not expect this problem with 2um tin-
lead.

Can you do the following:-
Minimise undercut by using thin copper foil
Optimise etching parameters- (<8.5 pH in ammoniacal etch - 8.2 optimum)
Plate the tin-lead as thin as possible - (3-4um should be okay).

One final thought,if your trace edges are not covered with solder after
fusing, you are leaving more tin-lead on the surface. Check the solder
conditioning and fusing flux.

Good Luck,
-- 
Paul Gould
Teknacron Circuits Ltd
[log in to unmask]
Isle of Wight,UK

***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]>   *
* with <subject: subscribe/unsubscribe> and no text in the body.          *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact   *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask]      *
***************************************************************************


ATOM RSS1 RSS2