TECHNET Archives

February 2011

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Douglas Pauls <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Tue, 1 Feb 2011 11:40:51 -0600
Content-Type:
text/plain
Parts/Attachments:
text/plain (114 lines)
Michael,
I will give it a shot.

1)  Documented, as in a standard "thou shalt use DI water"?  Not really, 
no.  It would be considered as a Best Manufacturing Practice though.  Most 
standards and specifications are based on the theory of we don't care how 
you clean it, it just has to meet "X". 

2)  Chloride on electronics is as common as nitrogen in air.  The issue is 
how much is present and how free is the chloride to react and do its dirty 
work.  What method did you use to determine chlorine contamination?  I 
know it takes quite a bit to make gold electromigrate.  In your case, ROSE 
is worthless, worthless I tell you.  You need to have your bare boards 
analyzed by ion chromatography in their incoming state, and your 
assemblies tested by ion chromatography after your city water cleaning 
process.  That will tell you where your chlorides are coming from and who 
to go after when you arm the villagers with torches and pitchforks.  You 
can do the same thing on components in the incoming state to see how much 
they contribute to the picture.

3)  Is 80-100 psi too strong?  Depends.  Do you want components on the 
board when you are done?  I would suggest a lower pressure, but a higher 
volume.  Mike Bixenman of Kyzen Corporation gave an excellent paper on 
this at the IPC Cleaning and Coating Conference in December.

Doug Pauls



"Forrester, Michael (H USA)" <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
02/01/2011 11:08 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Forrester, Michael (H USA)" <[log in to unmask]>


To
[log in to unmask]
cc

Subject
[TN] PCBA Water Wash






I have three questions I hope someone can help me with:
 
    1) We have a vendor that uses "city water" directly into their SMT
PCA washer.  I believe DI water is industry standard.
    Does anyone know if it is documented anywhere?  Spec?
 
    2) We had an issue where there was Chlorine contamination and gold
dendrites found inside some standard gull-wing 6 pin SMT ICs.
        This issue seems to be batch related.  The chip manufacturer
claims that chlorine is never used in their process.  Should the SMT 
        process expect to handle the possibility that the wash solution
may get into a part? The PCA vendor uses unfiltered "city water", 
        with no cleaner, in the wash process and does a ROSE test on one
board of each lot.  Since the ROSE test passes, the PCA vendor 
        is blaming the part manufacturer for having "leaky" parts, since
the thinking is the wash is getting into the part and trapped. 
    3) One issue I have is the water pressure in the wash is 80-100 psi.
I think this is too strong, and should be half of that?  You want to 
        flood the board with water, not hit the board and bounce off?
 
    Thank you in advance.
 
Best Regards,
 
Michael Forrester
Sr. Product Engineer
 

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site 
http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional 
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 
ext.2815
-----------------------------------------------------



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2