Hi "boardmanusa,"
You do not say what kind of BGA, whetherSMD or NSMD, how close the failures
are to the SJ interface. If good wetting has taken place ( failurs are not
interfacial) you may have SJ fractures due to thermal shock (=cooling too
rapid after reflow). The larger the component the worse this gets.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 904-437-8747, Fax: 904-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|