Linda:
Actually, it is quite possible to get black immersion Tin. It comes from running a bath with an excess of Cupric Copper in it. I wrote a article on how to monitor Cupric Copper in immersion Tin baths to avoid this in a recent PCD&F magazine.
The black color should not affect solderability, as it is actually immersion Copper on top of the Tin.
Rudy Sedlak
RD Chemical Company
--- On Fri, 9/18/09, Linda Langley <[log in to unmask]> wrote:
From: Linda Langley <[log in to unmask]>
Subject: [TN] Black Pad
To: [log in to unmask]
Date: Friday, September 18, 2009, 3:12 AM
I know we have had this subject many times before so I did go to the
archives and still can't find an answer. My question, is Black Pad only
associated with ENIG? Is it possible with immersion Tin?
Linda Langley CIT
Training Specialist
Jabil Circuit
248-292-6176
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|