Good point, Vladimir.
Possibly Gilbert's boards are displaying nickel skips due to bromide contamination just prior to plating.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Igoshev, Vladimir
Sent: Tuesday, April 15, 2008 10:57 AM
To: [log in to unmask]
Subject: Re: [TN] SV: [TN] Non wetting problem
That is why I asked for the original spactra. Don't you thing it's strange that neither Ni, nor P (if it's ENIG) were mentioned in the original e-mail?
Regards,
Vladimir
----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Tue Apr 15 11:51:46 2008
Subject: [TN] SV: [TN] Non wetting problem
Probably best on this is Rudy Sedlak or other guy from the chemistry bransch. I think you may have to do with Nickel-Bromide, which is sometimes used for the barrier layer.
Inge
-----Ursprungligt meddelande-----
Från: TechNet [mailto:[log in to unmask]] För Richard Kraszewski
Skickat: den 15 april 2008 04:56
Till: [log in to unmask]
Ämne: Re: [TN] Non wetting problem
Some quick thoughts before I call it a day?
Br- Possible something from the FR4fire retardant? Dust from routing?
Non-wetting? Well you can plate onto about anything (ie., bronze baby shoes). Perhaps the gold is thin and dissolves quickly exposing an unsolderable (highly oxidized) surface beneath?
Rich K / KEJ
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Gilbert Min
Sent: Monday, April 14, 2008 9:48 PM
To: [log in to unmask]
Subject: [TN] Non wetting problem
Dear All.
Hope you had a nice weekend.
I got a call from my customer that my PCB has non wetting problem, and I received 2 defect samples
I saw the contaminated gold plated surface @ 1st sample, no abnormal surface and defects were found @ other sample.
I understand the contaminated gold surface was able to make non wetting problem, but Another sample, I couldn't find anything on surface.
We did FE-SEM / EDX analysis.
Results: 1st sample: Br, Au, C, O, Au
2nd sample C, O, Au Ion were detected
.
I wonder why Br was detected?, do you have any idea for defection of Br on Gold plated surface?.
For 2nd sample, I have no idea, I could not understand the mechanism for non wetting problem without any abnormal gold plated surface.
If have idea & possible, would you share your great wisdom to me?
Best Regards / Gilbert Min
Tel.: 82- (0) 11-9242-5340
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|