Hi Technos,
I'm in big trouble with a backplane.
It's a 13.5"x19.5", 3.7mm thick. The connectors are disposed in parallel
lines, forming two columns a the two extremities. In the middle we have no
components. In between the connectors there are some TH caps and resistors.
______________________________
______ ______ I
______ ______ I
______ ______ I
______ ______ I
.. ..
..
______ ______ I
_______________________________ I
For a long time the soldering was OK, with small problems in the four
corners ( a couple of holes not 100% full).
For about a week or so, the solder joints of many caps or resistors present
cold solder. There are no significant cold solder problems with the
connectors, which present though a little less wetting (some of the fillets
are not what they used to be).
The question is: why do I get the cold solder and how can I get read of it?
We use :
- no-clean technology
- Multicore Sn63 solder
- Multicore X33 flux
- strong radiation preheating ( two top preheaters at 700F and two bottom at
750F); we spent a lot of time tweaking to avoid damaging the board
- two passes, one for fluxing only, no wave, the second one right after with
no fluxing, but with wave
- no chip wave (that's what I have, hehehe), just omega on our Electrovert
Econopak II
Any help would be greatly appreciated.
Thanks, Ioan
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|