Hey Rob,
Several areas to look at.
* Ensure that the nitric acid concentration is >30%v/v, more
preferably ~70%v/v. How old and what is the concentration of the current
acid. If it has a lot of nickel or is low in acid, it will not properly
passivate the SS (i.e. You will not form the passive oxide film)
* Have there been any incidences in the past where the system has been
left on during nitric passivation? In this case, the tank has been etched
and will not form a passive regardless of what is done to it unless it is
re-electropolished.
* If the EN bath or its components have been sitting around for some
time and have lost some of their stabilizers, you will see a less stable
passivation system since the EN bath will have a stronger tendency to want
to plate out and will tax the system more. This is attributable to the EN
chemistry.
* Has the mix of work changed? Some substrates can influence the
stability of bath through leaching out of certain compounds or excessive Pd
adsorption.
* Has the chemistry been maintained within close limits? Large swings
will tax the system more.
* Has the tank been damaged by scratching, etc? This prevents
formation of the protective oxide film in these areas.
* Are the cathodes actively plating in the EN? They should be.
* Make sure the cathode bar is not being forced against the tank wall by
solution movement. A poly spacer bar can be added to the bottom of the
cathode.
Hope this helps,
Best Regards,
Rob Durante
OMG Fidelity
Southern California
(714) 540-7388
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Russell Burdick
Sent: Tuesday, January 30, 2001 7:48 AM
To: [log in to unmask]
Subject: [TN] Anodic Protection of Electroless Nickel
Hello Everyone,
Perhaps any operators of an anodic protected electroless nickel bath can
help a brother out?
System has been up and running for about 10 months; problems with plate out
onto steel liner in the last 2 months. After passivating and stripping
nickel with nitric acid solution bath and anodic protection works fine for
about 3 operating days, then current flows above 1.5 amps and plate out
ensues (at this point the current increases as the bath temp increases).
I have contacted device manufacturer and the chemistry vendor, but would
appreciate any suggestions from my colleagues.
Thanks in advance,
Russell Burdick
Process Engineer
602-276-1600
_________________________________________________________________
Get your FREE download of MSN Explorer at http://explorer.msn.com
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|