TECHNET Archives

November 2000

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
"Ingemar Hernefjord (EMW)" <[log in to unmask]>
Date:
Wed, 29 Nov 2000 09:16:18 +0100
MIME-Version:
1.0
X-To:
Mike Fenner <[log in to unmask]>
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "Ingemar Hernefjord (EMW)" <[log in to unmask]>
Parts/Attachments:
text/plain (140 lines)
As far as I understand, a good rule for getting a good solderability is to use the 'wet-on-wet' method, i.e. the nickel must be followed of next steps instantly, not waiting for next hour. Too simple?
Ingemar

-----Original Message-----
From: Mike Fenner [mailto:[log in to unmask]]
Sent: den 28 november 2000 20:47
To: [log in to unmask]
Subject: Re: [TN] Ni/Au solderabilty


Random problems are hard, but to jargonise there is an "uncontrolled
variable" in the line, eliminate all the uncontrolled variables and
the problem will go. I would be looking in rinse and drying areas as
something is being carried forward to contaminate the pads.
We can assume they have double checked all their process chemistry by
now and found it to be OK so you are looking for things which get
overlooked eg, this problem could be caused by oil in the air lines
used for blowing dry, unauthorised silicone coming off conveyor chain.
IF none of their other customers are reporting problems then of course
these things could be going on in your own site......


BOL

Mike



----- Original Message -----
From: "Burtt, Nigel" <[log in to unmask]>
To: "'Mike Fenner'" <[log in to unmask]>;
<[log in to unmask]>; <[log in to unmask]>
Sent: Tuesday, November 28, 2000 9:16 AM
Subject: RE: Ni/Au solderabilty


>
> Thickness and porosity have been checked by the supplier and claimed
to be
> OK. Naturally we are discussing the matter in earnest with the
supplier, the
> problems are random, not on every board or batch so we don't find
out until
> after the boards leave the reflow oven! Pre-screening for
solderability will
> not definitely catch the problem.
>
> > -----Original Message-----
> > From: Mike Fenner [SMTP:[log in to unmask]]
> > Sent: Monday, November 27, 2000 5:08 PM
> > To: Burtt, Nigel; [log in to unmask];
[log in to unmask]
> > Cc: James, Chris
> > Subject: Re: Ni/Au solderabilty
> >
> > Nigel, The usual cause of poor solderability of Au over Nickel is
> > passivation of the nickel.
> > The most common reason for this - assuming boards are not out of
> > time - is the Au being too thin or porous.
> > The next most common is the nickel is already passivated at the
time
> > of application of the Au.
> >
> > [Keep in mind the Au plating does not enhance the solderability of
the
> > Ni, the best it can do is keep the Ni in the same condition as
when it
> > was applied.  The worst it can do is to shield the Ni from any
> > attempts to correct the problem.]
> >
> > In either case I am not sure what you can do, other than to
understand
> > your supplier's problems. At the risk of sounding a little harsh
why
> > do you want to take this problem on anyway? The boards are either
to
> > your specification and functional requirements or they aren't. You
> > naturally have a spec which calls out optimum plating thicknesses
and
> > you have a solderability test included to ensure functionality, so
> > what do you need to do if work is found to be out of spec or
> > non-functional and non-correctable?
> >
> > Mike
> >
> > ----- Original Message -----
> > From: "Burtt, Nigel" <[log in to unmask]>
> > To: <[log in to unmask]>; <[log in to unmask]>
> > Cc: "James, Chris" <[log in to unmask]>
> > Sent: Monday, November 27, 2000 10:16 AM
> > Subject: Ni/Au solderabilty
> >
> >
> > > Anyone out there got more than their fair share of problems with
> > > solderability on PCBs with electroless Ni/Au surface finish at
the
> > moment?
> > >
> > > We have had problems before from a supplier, with Ni/Au boards
> > poorly dried
> > > after the final rinse and others with copper contamination in
the
> > acid clean
> > > bath, but this looks like it might be a new cause. Phosphorous
> > content does
> > > not seem to be relevant.
> > >
> > > Thanks
> > >
> > >
> > > Nigel Burtt
> > > Production Engineering Manager
> > > Dolby Labs Inc - European HQ
> > > Email: [log in to unmask]
> > > Tel:     +44 (0)1793 842132 [direct line with voicemail]
> > > Fax:    +44 (0)1793 842101
> > >
> > >
> > >
> > >
>

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2