I am in the middle of an issue concerning a high temperature Laminate
and low pull force copper pads. The copper can be pulled from the PWB
with low pull forces and are failing in the field.
I have examined multiple damaged PWBs and have found that in ALL cases
the damage is the failure of the copper to epoxy bond. A good PWB will
normally fail within the laminate material.
The units are built using Pb-free processes with Pb-free components. I
am trying to determine what can be done to show that the laminate is not
good or in the PWB manufacturer did not laminage the layers correctly.
I do not have easy access to bare PWBs that have not been processed.
Any help or direction would be welcomed.
Thanks,
Mark
mark
Mark Woolley |PTRL Laboratory | Avaya | 1300 West 120th Ave |
Westminster, CO 80234 USA |
Voice (Lab): (303) 538-2166 | email: [log in to unmask] |
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|