TECHNET Archives

January 2008

TechNet@IPC.ORG

Options: Use Proportional Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Bev Christian <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Bev Christian <[log in to unmask]>
Date:
Fri, 18 Jan 2008 18:43:59 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (104 lines)
:) Inge I've known you for 10 years and I STILL think you are both brilliant and weird. 

Have a great weekend. 
Bev

----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Fri Jan 18 18:18:04 2008
Subject: [TN] Solderability of Tin-Gold Intermetallic, summing up

So, this is the conclusion: Bev woke up with head in someone's pillow, when
he startled in confusion, the balls were pried off. He consulted TN docs for
a diagnosis, however, they did not see the whole picture, but did as docs
use to do: only looked at the bad organ instead of whole symptom. Bev
insisted there is nothing wrong with the balls, instead one should
investigate the pillow. Docs consulted each other, and, cautiously, proposed
the problem may be in Bev's head. Others suspected something was left on the
pillow, but what. If there was gold, which seemed unlike, it could come from
the balls, but many docs claimed that heavy metals like gold is normally not
accumulated in the balls. So, again, the docs had a discussion about the
pillow. Could the gold come from the pillow?  Golden pillows are generally
only seen with elderly women (they can be very well done).The discussions
went on, but ended in total disorientation. Finally, the docs did not see if
Bev had head or balls on the pillow. The ordination became very odd: Bev,
next time heat is on, don't bother about the wetting, let your fantasy play
with 'golden balls' it's OK, all will work if you just have the process in
an atmosphere that suits both parties, and stop having the head in a cushion
at the same time.

Still Friday..and Bev will kill me..

Inge

-----Ursprungligt meddelande-----
Från: TechNet [mailto:[log in to unmask]] För Werner Engelmaier /*
Skickat: den 18 januari 2008 21:43
Till: [log in to unmask]
Ämne: Re: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold Intermetallic

Hi Bev & All,
I do not know why nobody responded to my e-mail. I said:
"Just like George, I am struggling getting an understanding of you problem.
To me, 'head-on-pillow' solder defects are almost always caused by 
insufficient peak temperature.
If these HOP's occurred essentially near the center of the BGA, you have
your 
answer,
If the HOP's are distributed over the whole array, than the root cause is
not 
insufficient peak temperature unless the whole reflow process is too low."

I am still betting on insufficient peak temperature. HOP implies a large 
pasty range; thus your solder(s) are not near eutectic. Whatever alloy they 
actually are, the insufficient peak temperature was too low to get them
fully liquid 
to join up.

Werner



**************
Start the year off right.  Easy ways to stay in shape.
     
http://body.aol.com/fitness/winter-exercise?NCID=aolcmp00300000002489

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2