Hi Bob,
Yes, it is definitely at the interface, right where the IMC is.
The pads are ENIG and have been cleared of any contaminants by EDAX.
The cracks completely shear the component off the board in one assembly
which had a bit of stress due to mask defined apertures which were
accidently reduced.
On another assembly the cracks only penetrate three balls in from the
outside (currently....).
Phil
At 03:28 AM 2/13/2008 -0800, bob wettermann wrote:
>Dear Phil:
>
>1. Have you done a dye and pry and confirmed that is indead the ball/board
>interface?
>
>
>2. Have you completed an analysis of the pad to determine what if any
>constitutes are o the pads?
>
>3. Are the cracks or opens across all areas of the BGA or just corners or
>one area?
>
>Bob Wettermann
>BEST
>Phillip Bavaro <[log in to unmask]> wrote: I am wondering if
>anyone else out there has run into a problem with a
>Samsung Flash memory device (in this case, the 0.8 mm pitch, 107 pin sac305
>BGA) where the connections are cracking right at the interface between the
>pwb and ball.
>
>I had read about some Samsung BGA problems but cannot find the link to the
>information now.
>
>We have other BGA's on the same board without any issues. Shear strength
>test results are very low as well (if the flash has not already popped off
>by itself).
>
>I'll try to get some pictures to Steve to put up tonight. My current
>thoughts are CTE's are grossly mis-matched as we haven't found anything on
>the pads to account for the gross failure.
>
>Thanks in advance,
>
>Phil
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
>
>
>
>Bob Wettermann
>PH 847-767-5745
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|