Hello! I recommend you conduct a solderability test in accordance with the
IPC JSTD-003 specification. The issues you describe are root caused in the
plating process and you can demonstrate to your ribbon manufacturer that
the wetting is not acceptable per a consensus standard and that there is a
need to correct the situation. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
[log in to unmask]
Sent by: TechNet <[log in to unmask]>
11/10/2010 12:58 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]
To
[log in to unmask]
cc
Subject
[TN] Question on ENIG process
Hello technetters.
We have a bad wettability (SnPb process) on some copper ribbons covered by
a Ni layer and Au layer. These are applied by an ENIG process.
The ribbon no-wet area is located on alongside and edges of ribbons. No
issue in the centrum area of the ribbon. The ribbons are 3 mm width and
0.3 mm thick.
The Ni layer and Au layer have the good thickness : 4µm and 0.1 µm. But
with a SEM analysis we see in the bad area a porous Au.
At the degolding operation, the area becomes black, the SnPb don't wet
and the SEM analysis gives a high presence of Phosporus in that area
(Qualitative analysis, the P peak is half the Ni peak).
At soldering operation more you try and worse it is.
The manufacturer of the ribbon says the P in the Ni-P bath is 9%.
Question:
I think the cause is a bad control and homogeneity of the Ni-P bath. Is it
correct or could be another cause as "only" 2/3 of the lot is bad?
After ENIG process, how many P has to remain on the Ni layer ?
Thanks for your answers.
Best regards,
CANTAGALLO Luigi
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|