Thanks to everone, I never realized there was so much support from so
many.
We are yet working on the situation. Thanks again.
P. Lance Mayes
Mfg. Trainer
Bev Christian <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
09/03/03 07:01 AM
Please respond to "TechNet E-Mail Forum."; Please respond to Bev Christian
To: [log in to unmask]
cc:
Subject: Re: [TN] pic's
Lance,
Well for a first timer, you sure got a lot of responses! Good first
question!
I have gone back and reread you original query, Howard's expansion and all
the replies. So what do we know:
1) Applies to ON Semi diodes only
2) Happens on secondary side
3) Parts pass solderability testing
4) Only happens on one of the two leads on the part
5) Chain conveyor and there are cooling zones
6) Happens "inconsistently"
I doubt very much you have a cold solder joint.
We definitely need answers to Werner's questions as to the orientation of
the parts and is it always the trailing lead (if this is the orientation)?
Is there a difference in CTE between this part and equivalent parts from
other suppliers? What is the difference between the heat sinking abilities
of the different pads to which the part is soldered? If it is a disturbed
joint on these parts but not others, the presence of a CTE difference,
with or without additional heat sinking, is the only reason I can come up
with so far to explain the difference.
If it is not a disturbed joint and the condition is truly random, then I
would wonder whether:
1) ON Semi got a questionable lot of lead material feedstock/solderable
surface with a SMALL amount of impurities in the metal(s,) which are
showing up on the surface of the joint (but not enough to affect
solderability testing - if so, who cares?)
2) The slight difference in cooling of one end compared to the other (heat
sinking, thermal shadowing) is allowing slight differences in surface
morphology that gives different light reflection properties. On TechNet
we have received several questions about rainbow, iridescent colors on
solder joint surfaces and that's all it is.
Keep digging, Lance, and let us know more! I am very curious to see how
this plays out.
regards,
Bev Christian
Research in Motion
-----Original Message-----
From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: September 3, 2003 7:55 AM
To: [log in to unmask]
Subject: Re: [TN] pic's
Hi Lance,
I would venture to say, that the CTE of these diodes is significantly
different than the PCB. I would further hazard the guess, that the diodes
with
disturbed SJs are predominantly those oriented in the conveyor belt
direction. What
I think is happening is that the leading edge SJ solidifies, the trailing
edge one is still pasty, and the differential contraction on cooling
causes the
trailing SJ to be disturbed.
Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|