TECHNET Archives

April 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Tue, 26 Apr 2005 09:46:10 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Vladimir Igoshev <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="utf-8"
From:
Vladimir Igoshev <[log in to unmask]>
Parts/Attachments:
text/plain (201 lines)
Victor,


What features  do you want to etch it for?


Vladimir
Sent from my Blackberry Wireless 
Vladimir Igoshev, 519-888-7465 ext.5283


-----Original Message-----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Tue Apr 26 09:42:48 2005
Subject: Re: [TN] Lead Free, Ball Grid Array, solder bump cross section

George,

   I did resolve my polishing artifact issue.   It was all in the water
/IPA rinse.

Do you know of a chemical etchant for LF solder?

Thanks for you input.

Victor,

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
Sent: Monday, April 25, 2005 4:04 PM
To: [log in to unmask]
Subject: Re: [TN] Lead Free, Ball Grid Array, solder bump cross section

Victor,

We use MasterPrep all the time and don't see the problem you are
referring to.  As Wade indicated if there is separation between your
sample and mounting material, or for that matter if you have lots of
voids in the solder joints you will trap water and polishing compound in
the separation or voids that well come out slowing and mess you nicely
polished surface up. 

Regards,
George
George M. Wenger
Reliability / FMA Engineer
Base Station and Subsystems Group
Andrew Corporation, 40 Technology Drive, Warren, NJ 07059 (908) 546-4531
[log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of McFaddin, Wade
Sent: Monday, April 25, 2005 4:51 PM
To: [log in to unmask]
Subject: Re: [TN] Lead Free, Ball Grid Array, solder bump cross section


Hi Victor,

We use a colloidal silica solution (0.05 micron) for our final polish.
We
polish for about one and a half minutes, with the final half minute
running
water on the cloth (Buehler's micro-cloth) and cross-section. This
cleans
the cloth and the cross-section mount of the colloidal solution. We then
rinse just the cross-section mount again with water and then quickly
rinse
with alcohol (IPA) and blow dry with nitrogen and wipe lightly with a
cotton
ball.  This usually gives us a clean, stain free surface. However, if
you
have pull-away (separation) of your mounting epoxy to the sample
surface, it
can be very difficult to get all the water and polishing solution out of
the
separation area.

Hope this helps.
Wade McFaddin
Nextek Inc.

-----Original Message-----
From: Victor G. Hernandez [mailto:[log in to unmask]]
Sent: Monday, April 25, 2005 1:48 PM
To: [log in to unmask]
Subject: [TN] Lead Free, Ball Grid Array, solder bump cross section

Fellow TechNetters:

   I have conducted many of LF solder bump cross section and final
polish is conducted with a Buehler Masterprep

Polishing Suspension Alumina 0.05 microns.   Micro craves, epoxy
shrinkage/voids, on the sample surface retain

the polishing compound which contaminate the surface appearance.   This
step can cause staining and/or water

marks on the bulb solder prior to mid range magnification examination
with inverted stage microscope.

   Can some one recommend a LF chemical etchant that I can replace the
alumina step in my process?

Victor,




---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

------------------------------------------------------------------------
------------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.  
If you have received it in error, please notify the sender
immediately and delete the original.  Any unauthorized use of
this email is prohibited.
------------------------------------------------------------------------
------------------------
[mf2]

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------




---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2