Russell,
Sounds as if you might have more than one issue here.
Regarding the dull solder joints: How does the gold thickness of the May
and October batches compare? (Note: use measurements taken after the May
boards were scrubbed) The treatments given to your gold bath could increase
plating efficiency and/or alter the surface finish of the nickel. Gold
plating is usually so thin that it mirrors the surface of the underlying
nickel. If the October batch is thicker, your customer may be seeing a
gold/solder alloy. I don't know the concentration where the appearance
changes (seems like 30 microinches is a magic number), but gold
embrittlement could be an issue.
Regarding the inability to recognize fiducials: Scrubbed gold has a
different surface texture that plated gold. Even though they appear shiny,
the different textures can fool the cameras. An eraser could "fix" the
problem until the cameras are adjusted for the new surface condition.
Just a quick note: black pad is not associated with electrolytic plating.
Hope this helped.
Don Vischulis
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Russell Burdick
Sent: Thursday, November 14, 2002 4:04 PM
To: [log in to unmask]
Subject: [TN] gold solderaility
Hello everyone!
I could use some help concerning soldering to gold.
Problem:
A customer of ours has given feedback to our salespeople that hard gold
boards we made in May 2002 were much better to solder to than what we sent
in October 2002. Biggest difference was stated as the newest boards have
fiducials that auto pick and place equipment can't read because under the
lights they look "black". Under normal shop lights both boards look bright
and shiney(sp?).
Also, the customer commented that on the boards with "black" unreadable
fiducials had solderjoints that looked very dull.
Known manufacturing/processing differences between months of May and October
(aka, confessions of a process engineer):
Prior to August 2002, dull plated gold boards were scrubbed to improve
appearances. After August 2002 no scrubbing needed when a carbon treat and
proper wetters were performed/maintained in nickel and gold baths.
Any and all comments are greatly appreciated.
_________________________________________________________________
Help STOP SPAM with the new MSN 8 and get 2 months FREE*
http://join.msn.com/?page=features/junkmail
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|