Hi, I am going to put my 2 cents worth in. This might apply to the messages
about ancient design issues as well. I remember working at the EMPF in Indy
and a gentleman from England that had a concept of putting on material
(build up) around through holes that would come off the wave without a
complete fill. The concept had to do with thinking the solder wave was
water and by causing turbulence (damming) affect the hole would then fill.
He used an example of a connector pin that would not fill but after adding
the material it would fill every time. I cannot remember his name but his
idea came to mind this morning. He was a Cat B (if some of you might
remember that from the WS-DOD-Mil days). Maybe some of you can remember his
name or concept. The material could be add and removed or be part of a
redesign. PS I have always believed the Cat A, B, C, D, E, R that was used
was from the "Cat in the Hat" book. Jon
-----Original Message-----
From: Stephen R. Gregory [mailto:[log in to unmask]]
Sent: Thursday, August 10, 2000 1:00 PM
To: [log in to unmask]
Subject: [TN] Topside solder fillets after wave...
Hi all!
Been trying to dial a profile in on the wave today with a board that's
fairly
thick, probably around .090", polyimide, all PTH with a fair amount of the
IC's being ceramic. We use a spray fluxer and a RMA flux.
The first boards have been coming off without the preferred topside fillets
at a number of locations. I've been playing with the pre-heat, belt speed,
and even did something that I don't like to do, which was to flux the
topside
of the board.
All to no avail...I still had quite a few places that didn't have topside
fillets, and that is something that doesn't go over well here at all.
I started noticing that the places that didn't have topside fillets were at
the same locations. So I came back to my 'pooter and looked at the gerber
for
the board. What's really weird was that everyplace there's a thermal for a
pin is where I have no topside fillet??? I thought that thermals were
supposed to help prevent that from happening? But it's true, every single
place there is a thermal= no top solder. Has anybody ever seen that before?
-Steve Gregory-
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|