Ken:
One thing you should probably keep in mind - I don't think you
really have the option to "check the torque after torquing".
Try this - tighten the screw with controlled torque (crank on the
torque driver until it slips), then take a torque watch and
measure the torque required to loosen the screw.
The "breakaway torque" is always much higher than the original
torque applied, because once the screw stops turning, you
start dealing with static friction, galling, micro-welds. And
because most of the effects are non-linear, breakaway torque
doesn't look very repeatable.
-Joe
-----Original Message-----
From: Hal Winslow [mailto:[log in to unmask]]
Sent: Wednesday, March 17, 2004 10:41 AM
To: [log in to unmask]
Subject: Re: [TN] Torque Stripe
I seem to remember some calibratable torque drivers that would automatically
apply a paint mark after they tightened the hardware to whatever set point
you had. Accomplishes everything in one quick operation.
Unfortunately I can't remember the brand that offered this option, but if
you start chasing down some of the more "luxurious" versions of torque
drivers I bet you will find this as an option.
Good Luck,
Hal
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Bloomquist, Ken
Sent: Wednesday, March 17, 2004 10:24 AM
To: [log in to unmask]
Subject: [TN] Torque Stripe
Good Morning Technetters,
We have a new program in house where the customer is asking us for torque
verification on some hardware. I was wondering if any of you have some
clever ideas to make this an easy task. The obvious solutions are adding
some paint after torque, having someone check the torque after torquing and
having a witness while torquing. All of these are sort of painful.
By the way we are torquing phillips head screws.
Thanks for any thoughts,
KennyB
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|