TECHNET Archives

February 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Fri, 15 Feb 2008 22:46:44 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, David Tremmel <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
Subject:
From:
David Tremmel <[log in to unmask]>
Content-Type:
text/plain; charset="UTF-8"
In-Reply-To:
MIME-Version:
1.0
Comments:
RFC822 error: <W> MESSAGE-ID field duplicated. Last occurrence was retained.
Parts/Attachments:
text/plain (68 lines)
Hello,

Pardon, but I thought that it was liquidus plus 20 degrees for 5 seconds to ensure a good metallurgical bond.

So do you mean 

217 (solidus for SAC305)+ 20 + 15 = 252 for 5 seconds

or

221 (liquidus for SAC305) + 20 + 15 = 256 for 5 seconds?


Just want to make sure that I am not missing something!


Thank you,
 
David Tremmel

VALUE RECOVERY
Quality is the nature of the service

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /*
Sent: Viernes, 15 de Febrero de 2008 09:28 p.m.
To: [log in to unmask]
Subject: Re: [TN] Samsung Memory BGA Failure

Hi Phil,
Your T-measurement method is perfect—you IN FACT know what the T's are.
My recommendation for reflow soldering is:
Liquidus + 20C + (15 to 20C when soldering to NI) for 5 seconds minimum; thus 
in your case we have 217 + 20 + 15 = 252C for 5 seconds 
So, it is still likely you have not formed a decent metallurgical bond.



Werner



**************
The year's hottest artists on the red carpet at the Grammy 
Awards. Go to AOL Music.
      
(http://music.aol.com/grammys?NCID=aolcmp00300000002565)

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2