IPC-600-6012 Archives

October 2009

IPC-600-6012@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Werner Engelmaier <[log in to unmask]>
Reply To:
(Combined Forum of D-33a and 7-31a Subcommittees)
Date:
Fri, 30 Oct 2009 11:19:37 -0400
Content-Type:
text/plain
Parts/Attachments:
text/plain (66 lines)
 Hi Pete,
What you are seeing are conductive anodic filaments (CAF) aong separations between the glass fibers and the resin. Started as  a less than perfect drilling of your PCBs and propagated in T-cycling [severe].
Werner

 

 

-----Original Message-----
From: [log in to unmask]
To: [log in to unmask]
Sent: Fri, Oct 30, 2009 10:34 am
Subject: [IPC-600-6012] Latent defects on PWA













All:

I have run into an anomaly that I am having trouble understanding. I am
including a couple cross section pictures to show the anomaly.

After as few as one thermal cycle (-55 to +60C) the boards are failing.
The failure is a reduced resistance between isolated circuits.  The
board shown in the pictures was  160 ohms.

I had the failed connection cross sectioned (both horizontal and
vertical views)  and it revealed a crack in the prepreg.  This is a 14
layer board and the crack is showing up between layers 7 and 8 - it is
B-stage that is cracking.  The laminate is polyimide.

As seen in the cross section pictures it appears to me that the crack is
happening after plating - most likely during my thermal cycle.  I see no
evidence of plating or any contamination in the crack. 

So, my question boils down to why is the crack manifesting itself as a
short or reduced resistance?  Has anyone ever come across something like
this or have an explanation?

Thanks for your help.

Pete Menuez 
Supplier Quality Engineering Manager 
L-3 Communications Cincinnati Electronics 