DESIGNERCOUNCIL Archives

November 2012

DesignerCouncil@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
DesignerCouncil <[log in to unmask]>
X-To:
Designers Council Forum <[log in to unmask]>
Date:
Tue, 13 Nov 2012 15:16:53 +0000
Reply-To:
"(Designers Council Forum)" <[log in to unmask]>, "Byrne, Matthew J (US SSA)" <[log in to unmask]>
Message-ID:
Subject:
From:
"Byrne, Matthew J (US SSA)" <[log in to unmask]>
Content-Type:
text/plain; charset="utf-8"
In-Reply-To:
Content-Transfer-Encoding:
base64
MIME-Version:
1.0
Parts/Attachments:
text/plain (1 lines)
Pete just described key features that are very close to IPC-4101/126.  This is one of the newer materials that IPC added to 4101 in the last revision

Another key product feature included in the /126 slash sheet is time to delamination, varying by the test temperature, but a good laminate should be able to pass 30 minutes at 260C before delaminating.  A good off-shore supplier will know and understand the IPC specifications.


Matt Byrne

-----Original Message-----
From: DesignerCouncil [mailto:[log in to unmask]] On Behalf Of Pete
Sent: Thursday, November 08, 2012 11:18 AM
To: [log in to unmask]
Subject: Re: [DC] PCB Material for Lead-Free RoHS

Kitty,

If this is s through hole board that will see one excursion through the wave, you can probably get away with the old 140Tg material ina  RoHS complaint form.

Tg as a spec is so old school now!  Some of the RoHS complaint 170Tg materials actually degrade to 130 and below after the first heating cycle.  

You need to also spec Td, and Z axis expansion.  And some multifunctional epoxies required to meet these specs can vastly increase the risk of cathode-anode failures (CAF).  So specify CAF resistant epoxy, or specify non-dicyandiamide epoxy (this is a common CAF resistant type)

So if your boards will be reflowed, especially if they will see more than one thermal cycle, try these specs:

LAMINATE MATERIAL SHALL BE IN ACCORDANCE WITH IPC-4101, EPOXY-GLASS LAMINATE, NON-DICYANDIAMIDE, NEMA GRADE FR-4, FLAMMABILITY RATING: UL 94V-0.
         MINIMUM Tg (DSC) 170
         MINIMUM Td (TGA) 330
         MAXIMUM Z-AXIS EXPANSION 25C-260C 4%   (you can alterrnately specify CTE, expressed as ppm/C)

And perhaps most importantly, if you are buying fabs overseas, make sure you use a good shop, don't just broker the boards.  Some have been known to completely ignore your specs and use whatever they can get cheapest.  Cheap isn't inexpensive when your yields drop and failures increase due to "cheap" fabs.  (Unless you are building "throaway" products)

Pete

---------------------------------------------------------------------------------
DesignerCouncil Mail List provided as a free service by IPC using LISTSERV 16.0.
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF DesignerCouncil.
To temporarily stop/(restart) delivery of DesignerCouncil send: SET DesignerCouncil NOMAIL/(MAIL)
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
---------------------------------------------------------------------------------

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________




---------------------------------------------------------------------------------

DesignerCouncil Mail List provided as a free service by IPC using LISTSERV 16.0.

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF DesignerCouncil.

To temporarily stop/(restart) delivery of DesignerCouncil send: SET DesignerCouncil NOMAIL/(MAIL)

For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

---------------------------------------------------------------------------------


ATOM RSS1 RSS2