Beware! Some of these products cause more harm than good. Prevention is better than cure. Use dross-free metal to start with. Dross requires oxide nuclei to form and, if the solder is free from oxides, dross formation will be slowed down. If possible, use an oil/polyglcol ether blanket, injected into or onto the wave. Never return a drossy solder to the bath. Occasionally, reduce the temp of the solder bath to exactly 186°C and keep it there, statically, for several hours, then skim the solder surface. This will help keep the oxides down, as the intermetallics, which oxidise readily, will be partially removed. Brian Ivan Barrios wrote: > What is an industry standard (or current experience) on dross produced > (relationship of adding new solder versus removing dross for, i.e. for every > pound of solder added we remove X amount of dross kind of deal) > Also, has anybody had any experience with using dross reducing agents (Kind of > like a detergent to sprinkle at removal of dross) to separate Good solder form > the oxides. I have acompany (no names ) that is trying to sell me on this stuff > and I would like to hear past experiences with this type of additives. > Any and all replies will be greatly appreciated > > Ivan Barrios > > ############################################################## > TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c > ############################################################## > To subscribe/unsubscribe, send a message to [log in to unmask] with following text in > the body: > To subscribe: SUBSCRIBE TECHNET <your full name> > To unsubscribe: SIGNOFF TECHNET > ############################################################## > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional > information. > If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or > 847-509-9700 ext.5365 > ############################################################## -- Brian Ellis Protonique SA PO Box 78 CH-1032 Romanel-sur-Lausanne, Switzerland Voice: +41 21-648 23 34 Fax: +41 21-648 24 11 E-mail: [log in to unmask] URL: Technical and consultancy divisions: http://www.protonique.com Web services division: http://www.protonique.com/webserv ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ##############################################################