Ryan,
Tin whiskering has been a problem with immersion tin. There however have been advancements in eliminating this problem. Atotech has added a step to the process which prevents the growth of whiskers.
Sincerely,
Don Janus
Eastern Area Manager
Electronic Chemistry
Atotech USA Inc.
Frank Freitas wrote:
Hello Ryan,
There are numerous suppliers of this process currently, each with their
strengths and weaknesses. I believe the greatest concern with immersion tin
as final finish however is with tin whiskering.
McGean-Rohco, Inc. (Cleveland, Ohio) has just recently presented a technical
paper at the IPC Works which covers this and has developed a solution to the
whiskering issue while at the same time allowing for immersion tin as the
final finish. If you would like additional information please contact George
Bokisa ( Technical Manager-Electronic Chemicals) @ 216-441-4900 in Cleveland
and he will gladly provide you any assistance you may need.Regards,
Frank Freitas
Technical Sales Engineer
McGean-Rohco, Inc.
2910 Harvard Avenue
Cleveland, OH
216-441-4900
------Original Message------
From: Ryan Grant <[log in to unmask]>
To: [log in to unmask]
Sent: November 3, 1999 7:42:27 AM GMT
Subject: [TN] immersion tin as a surface finishHi Technetters,
Anybody using immersion tin as a surface finish? What are some of its
quirks? We have a customer that wants us to use it, so we are going to
qualify it as soon as we can get some boards in from multiple suppliers.
During the qual, I would like to know ahead of time what problems to
look for. We are currently assuming it will be a drop in for our OSP
and immersion gold boards. (We got rid of HASL a while ago because of
shorting on fine pitch is orders of magnitude high than gold).Thanks
Ryan Grant
Process Development Engineer
MCMS
(208) 898-1145
FAX (208) 898-2789
[log in to unmask]##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################-----------------------------------------------
FREE! The World's Best Email Address @email.com
Reserve your name now at http://www.email.com##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################