I would also like to point out that ammonia can attack tin. I agree with the statements made in other responses about using a neutral cure RTV. I've used several from Dow Corning that work great and provide good corrosion protection by attaching to all (theoretically) sites that have oxidized. Good luck in fixing this problem. Aric Parr Sr. Process Engineer Eaton Corporation 1400 S. Livernois PO Box 5020 Rochester Hills, MI 48308-5020 248 608 7780 [log in to unmask] ---------- Original Text ---------- From: C=US/A=INTERNET/DDA=ID/TechNet(a)IPC.ORG, on 11/25/99 3:44 AM: Sherman There are a couple of points I'd like to make: 1. gold-plated Kovar is sheer hell (perhaps I should say shear hell!) for stress corrosion. I had some PCBs with gold-plated Kovar trannie leads (TO18) where the Kovar had totally corroded away where the leads had been formed, the connection being maintained by the gold, until the trannie fell off. This was in adverse climatic conditions. We got round this problem by solder dipping the leads up to 1 mm from the case after forming. I'm not saying this is the cause of your problems, which may be triggered partially by the presence of gold-tin intermetallics, but it's worth knowing. 2. RTV is about the worst kind of coating there is. Its chemistry is highly ionic and it requires atmospheric humidity absorbed to "complete" its polymerisation. Many types depend even on strong acetic acid to work. Also, ammonia + water = ammonium hydroxide, an aggressive alkali. Furthermore, although it is water repellent, it is the most humidity-porous of all coatings, some 20 times worse than epoxy coatings so, if you have any hygroscopic contaminant under the RTV, it will get nicely damp and stay damp, just ideal for creating corrosion, especially if it were ionic in nature, as could be with astoichiometric or incompletely cured RTV. My guess is that you need to qualify your process to your requirements. Brian Sherman Banks wrote: > Hi Technetters: > > I have recently joined this company and a legacy product has been having a > few field failures. The nature of the failure is a fractured solder joint. > It is a lap configuration of a Kovar (gold plated) lead onto a HASL SMT pad. > The fracture seems to originate at the point of the joint where the exposed > base metal is from clipping. The solder looks especially grainy although it > has not seen significant temperature cycles or time at temperature. > The solder joint is encased in RTV 128 as a conformal coating. According to > GE tech support, RTV 128 outgases ammonia as it cures. > My question is: Has anyone any experience using RTV in this situation? Has > anyone seen or heard about RTV attacking solder joints to this extent? > > As this is sent late on Thanksgiving eve, if you see it before Thursday, > Happy Thanksgiving, if after, I hope you had a Happy Thanksgiving. > > Regards, > Sherman Banks > [log in to unmask] > > ############################################################## > TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c > ############################################################## > To subscribe/unsubscribe, send a message to [log in to unmask] with following text in > the body: > To subscribe: SUBSCRIBE TECHNET <your full name> > To unsubscribe: SIGNOFF TECHNET > ############################################################## > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional > information. > If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or > 847-509-9700 ext.5365 > ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ##############################################################