Richard, I suspect that the holes in the area of the board that are not soldering properly are connected to the plane layers. This will cause them to soak up much more heat than the other holes. This can be checked with an ohmmeter, looking for continuity from the problem holes to power and ground. If this is so, suspect that this is one of the areas reaching a lower pre-heat temperature. If this is the case, you need to get the top-side tmep prior to hitting the wave to come up more. This can be done by slowing down the conveyor speed a bit. Another thing to measure is how long the board is in contact with the wave. If my memory serves me right, it should be about 3 - 5 seconds. The board also needs to go about 2/3 of its thickness down into the wave. You can look at the inside of the holes with a prism device and a backlight. That will give you some idea of the quality of plating/drilling in the holes. u see a buch of nodules and extreme roughness in the holes, then the board shop may have messed up the drilling/plating process. That may give you pin holes in the sidewalls, which will cause blow outs and/or blow holes in your solder joints. To me, it sounds like you main problem is not an even enough pre-heat across the board. Good luck, Charlie B. Richard Tilbrook <[log in to unmask]> on 10/26/99 03:05:31 AM To: Charles Barker/US/I-O INC@I-O INC cc: Subject: Re: [TN] HELP!!! - flow solder problems RT CHARLIE, PLEASE FIND BELOW THE ANSWERS TO YOUR QUESTIONS: Other folks have asked pertinent questions which I am not repeating here. You might want to look at the preheat temp.... What is the topside temp just prior to the boards hitting the wave? 85 TO 104 DEG. C - VARIES ACROSS THE BOARD. What kind of flux are you using and how is it being applied? ALPHA METALS 615-15 - RMA LIQUID FLUX (15% SOLIDS) SPRAY APPLICATION. Is it the same 4 - 5 holes on each board? THE 4-5 HOLES OCCUR IN THE SAME SMALL AREA. The the hole-to-lead diameter ratio big enough to allow the solder to flow/wick up the lead? WE AREN'T SURE. Is the solder just simply not flowing up the lead or is the solder being blown out of the hole due to outgassing due to contamination or pin holes in the plating in the holes? AGAIN, WE DON'T KNOW - WE DON'T MAKE THE BOARDS, AND WE CAN'T TEST FOR THESE WITH THE SUPPLIED BOARDS. These are a few things to check for. Good luck, Charlie B. THANKS FOR YOUR TIME, RICHARD TILBROOK BRITISH AEROSPACE ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ##############################################################