You dont say if this problem is all over the board surface, or just in certain areas. I once had experience of this problem in isolated areas of the panel, and found that the rubber coating on the rollers had bubbled slightly, (so slight, it was not visible to the naked eye), and the rotation and flexing of the rubber did not exert enough pressure onto the surface of the panel. New rollers did the trick, and the old ones sent for recovering. Another possibility, may be that the anti-tarnish process after electroless may not be rinsed off properly. Look for for tell-tale stains on the panels prior to lamination. Hope this helps Colin McVean Cookson Electronics At 11:22 12/07/99 +0200, you wrote: > > > >Dear Sirs, > >The reason why we send this e-mail is because we are having >problems of adherence of our dry film Dupont 4615. >The problem always appears beside the track/pads, and in the final pcb >you always can see a bigger track, because the adherence of the film has >not good and some Sn/Pb has get on the base copper (the film has not >protect correctly the base copper, beside the track). > >We have done the following corrective actions and there has not been >any success at all: >1. We have increased the lamination temperature from 105 to 115ºC. >The presion is about 4 bars. The lamination rolls speed is about 1,6-2 m/min. >2. We have checked the pH of the revelator solution and goes from pH >11 at the beginnig to 10,4 at the end of the solution live. >3. We are quite sure that is not a electrolitic line problem, because in the >same bath position, we have panels with and without problems. >4. We have checked all the insolation parameters and everything is OK. > >What we are doing now, is changing from Dupont film 4615, to 215. >Maybe, it will solve the problem, but we don't know the cause of our problem. > >Does anybody knows the cause of our problem ??? > >Thank you in advance for your colaboration. > >Albert Varon >Quality Manager. > > >********************************************************** >CIRCUITOS IMPRESOS PROFESIONALES,S.A.. >Pol.Ind.Els Bellots C/de l'Aigua, 28 >08227 TERRASSA (Barcelona) SPAIN >Apdo. de correos 597-598 >Telf. 34.937856793 Fax 34.937861905 >********************************************************** > > >Attachment Converted: "C:\TEMP\TNRVDryf" >