Hi Girlie, Here are a few quick thoughts: 1) check the quality of the artwork, i.e. the transition from dark to clear should be abrupt, 2) ensure that the artwork emulsion side is towards the dry film, 3) ensure that the artwork is in intimate contact with the dry film, 4) the dry film may be bad, try new rolls from a different lot, 5) check the exposure energy, over exposure will cause blooming, 6) check the exposure system for proper columniation, lamp quality, lamp on/off time, 7) take the day off and start fresh on Monday. Good luck, Tim Estes Conductor Analysis Technologies, Inc. Phone: 505-797-0100 Fax: 505-797-1605 Email: [log in to unmask] Web: http://biz.swcp.com/cat -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Girlie M. Austria Sent: Friday, July 30, 1999 7:55 PM To: [log in to unmask] Subject: [TN] Blooming problem Can anybody give me some suggestions on how to solve Blooming problem on dry-film imaging aside from the vacuum problem? Your help is appreciated. Girlie ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or 847-509-9700 ext.5365 ##############################################################