Kelly, et. al. Thanks for the information so far! I'm going to look into the C-SAM and chemical analysis Michael suggested. We're currently using adhesiveless base material on the parts due to some low yield problems we'd seen in the past. Unfortunately, the delamination we're seeing is coverlay to copper where we're using the acrylic adhesive. Does anyone have experience with epoxys or other adhesives for that component? As for the tweezer method, that's similar to what we've been doing as a check; I feel pretty good about the method, but I'm worried about the possibility of this discoloration, even if it doesn't give me the tactile delam feedback, having some problems later in life. I worried that even the C-SAM, while it can verify the parts as-is, won't necessarily tell me if I'll see any future problems (or if it's ok now, will it be ok in the future?). Does testing the bond strength between the cover and the copper help? This is something of a separate thread, but for adhesiveless flex materials, is there any practical functional difference between cast polyimide and sputtered copper (/11 and /12 I think). Is it a difference I should worry about when specifying materials? Thanks for the information so far! Matt Matthew Sanders PCB/Metal Procurement Engineer, Trimble Navigation Ltd. [log in to unmask] Phone: (408) 481-7817 Fax: (408) 481-8590 -----Original Message----- From: KELLY M SCHRIVER [mailto:[log in to unmask]] Sent: Tuesday, May 11, 1999 6:00 AM To: [log in to unmask] Subject: Re: [TN] Flex circuit - discolored copper, delam? Matt - From your description of the dark vs. light areas of copper, I suspect you are correct about a delaminated or debonded condition. The acrylic adhesive used in your flex has a glass transition (Tg) temperature of about 45C, as opposed to a Tg of 240-250C for the polyimide materials in the structure. This means your process temperatures can temporarily turn the acrylic adhesive to something rather like grease. In this state, it is subject to debonding/delaminating rather easily from any form of stress. I would suggest the following as a quick check to confirm: Place the specimen under low magnification (10-20X) and gently squeeze the suspect area with tweezers or similar. If debonded/delaminated you should be able to observe movement in the structure between the cover film and the circuit. Several years ago, DuPont, Sheldahl and others standardized and commenced marketing "all polyimide", "adhesiveless flex" or "bondable polyimide", or whatever you want to call it. This material has a Tg in the 230C or above range, which is much more durable. We have switched over most of our designs and have seen improved product yields at the fab houses and in our own assembly operations, as well. In our case, this has pretty well turned out to be a true "drop in replacement". All of our government sector customers, to date, have agreed that it is a class 2 change.. Good luck - I'm at 256.882.4536 if you need to talk. Regards - Kelly ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################