At previous employers and here I have used hard tooled solder pallets, water soluble paste, water soluble tape, masking tape, Kapton tape, plugs/corks, and liquid thermal or UV cure mask materials to mask pads on wave soldering. Have you tried removing the pad from the solder side of the panel, or making the pad less than 360 degrees? These usually prevent hole filling. Some water soluble tapes and pastes can clog filters in an in-line system, many don't. I dropped the concept when converting to no-clean and selling off the cleaners. Most tapes leave residues, many have silicone adhesives. I hope you don't need to conformal coat over the tape. Plugs/corks/toothpicks are very easy to use, but require labor and storage. Dedicated pallets work well for high volume parts. With the cost of pallets, you need considerable volume to cost justify vs. manual mask. Liquid and paste masks work well, but require curing time or an UV oven. They should be removed prior to any water wash or the water pressure will blow them off the panel and into the filter (or even into spray nozzles). ARIC PARR Sr. Manufacturing Engineer Eaton Corp 1400 S. Livernois P. O. Box 5020 Rochester Hills, Mi 48308-5020 [log in to unmask] 248 608 7780 Fax: 248 656 2242 ------------- Original Text From: C=US/A=INTERNET/DDA=ID/TechNet(a)IPC.ORG, on 5/25/99 7:52 AM: To: Aric Parr@01635@Lectron_RH, EatonWHQ@CorpMail@WHQCleveOH[C=US/A=INTERNET/DDA=ID/TechNet(a)IPC.ORG], Dean Jones@01635@Lectron_RH Kat, I have seen toothpick inside the trough-hole ( it is cheaper, you can use several times, fast placement / removal ) Thanks Jorge Dourado de Santana Maintenance / Process Engr Microtec - Brazil > -----Original Message----- > From: Kat Lee [SMTP:[log in to unmask]] > Sent: 25 de Maio de 1999 06:50 > To: [log in to unmask] > Subject: [TN] Plated Through-Hole > > Hello everybody, > This is my first time mailing to the list. > > I'll get straight to the point - you see, a product of my company has a > plated through-hole that must not be soldered. > The past solution was to cover the whole thing with a kapton tape before > running it through the wave. Now we have suggestions of using a plug or > water-soluble masking tape. > I was wondering if any of you have any experience in this matter and could > share anything with me. > > Thanks in advance. > > Kat LEE > > ################################################################ > TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c > ################################################################ > To subscribe/unsubscribe, send a message to [log in to unmask] with > following text in the body: > To subscribe: SUBSCRIBE TechNet <your full name> > To unsubscribe: SIGNOFF TechNet > ################################################################ > Please visit IPC's web site (http://www.ipc.org) "On-Line Services" > section for additional information. > For technical support contact Hugo Scaramuzza at [log in to unmask] or > 847-509-9700 ext.312 > ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################