Hi Jim! There is a fairly high probability the copper-tin crystallites you have seen are copper/tin intermetallics (Cu6Sn5 phase). There are some good studies in the industry literature by Morris, Yost, Romig, etc. showing that the Cu6Sn5 phase can be evenly distributed within a solder joint as a normal occurrence of the soldering process (there are some neat pictures of the phase as a hexagonal, hollow shaped geometry). Take a look in Klein Wassink's book for more info (ISBN 0-901150-14-2) pages 93-98. Good Luck. Dave Hillman Rockwell Collins [log in to unmask] Jim Marsico 516-595-5879 <[log in to unmask]> on 05/13/99 07:26:00 AM Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond to Jim Marsico 516-595-5879 <[log in to unmask]> To: [log in to unmask] cc: Subject: [TN] BGA FAILURE ANALYSIS Good Day Technet: First, a little background... We're in production using a 228 ceramic BGA for a military contract. The base material of the component is gold plated nickel, prior to solder ball attachment. The gold plating is very thin, around .25 microns. We've been experiencing approximately 5% (components, that is, not solder joints) open circuits found at in-circuit testing (ICT). Upon removal of the BGA (Air-Vac system) from the board, the specific ball location where the open was identified at ICT shows no solder remaining on the component, where all other locations has solder remaining. What does remain is a dull, gray, crystalline metallization. SEM/EDX analysis shows Ni/Sn and Cu/Sn. It is presumed that the Ni/Sn is the intermetallic layer created from the nickel base material and the tin in the solder. What puzzles me is the presence of the copper-tin crystallites. Since there is no copper in the solder or on the component, is it possible that this copper has migrated all the way up from the board pad to the component/solder interface? Thanks in advance... ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################