Sheila, I would first look at your flaring process. When I experienced this same problem in a previous life, I found that the operators were pressing the terminals too tight into the PWB. Of course, when the PWB heats up during the wave solder process, expansion occurs, thereby causing the stresses that you are seeing. What we found was that the terminals did not have to be tight before the soldering process. As long as the terminal could spin in the PTH w/o much z-axis movement, measling did not occur. Good luck. Rich Buccieri tyco Packaging Systems (Formerly AMP Packaging Systems) Phone:512.671.5555 Fax:512.671.5842 Email:[log in to unmask] > -----Original Message----- > From: Sheila Smith [SMTP:[log in to unmask]] > Sent: Tuesday, April 13, 1999 10:16 AM > To: [log in to unmask] > Subject: [TN] ASSEMBLY: measling around pressfit flared hardware > after wave solder > > Hi TechNet, > > We have a small multilayer (4, I think) GFG board which has 8 pressfit, > flared terminals installed along one edge, about 0.25" from the edge of > the board. After wave solder, these boards are being rejected for > measling around the hardware - typically between two terminals. The > measling was either not present before solder or was made more apparent by > the wave solder temperatures. The hardware is the correct size for the > board thickness and hole size & is being installed using the > manufacturer's tool. We did not observe this problem in previous batches > but the board material has been changed from FR4 to GFG [should have > helped, I'd think]. Is it possible we are doing mechanical damage to the > boards during flaring? Thanks in advance for your help! > > Sheila Smith, Marconi Aerospace > > ################################################################ > TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c > ################################################################ > To subscribe/unsubscribe, send a message to [log in to unmask] with > following text in the body: > To subscribe: SUBSCRIBE TechNet <your full name> > To unsubscribe: SIGNOFF TechNet > ################################################################ > Please visit IPC's web site (http://www.ipc.org) "On-Line Services" > section for additional information. > For technical support contact Hugo Scaramuzza at [log in to unmask] or > 847-509-9700 ext.312 > ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################