I just went thru that myself and here are my thoughts. An ionograph is OK for process control, if you use a high sensitivity one built for SMT cards. For process development, I actually removed a BGA and visually inspected it for flux residues. You could either use a clean BGA rework station, or a screwdriver. Prying the BGA off also gives some insight into the solder connections. You can see wetting, voids, blowholes, solder dam conditions, etc. (One could also measure the CCA and the removed BGA in the ionograph, as a more sensitive test.) Jim Kittel >-----Original Message----- >From: John Chandler [SMTP:[log in to unmask]] >Sent: Sunday, January 24, 1999 11:46 PM >To: [log in to unmask] >Subject: [TN] BGA clean checking > >As you all know. We are getting into doing a basic BGA assembly. The new >question which came up is, since we run a water soluble flux paste. How are >we going to know if it is clean under the BGA?? Any suggestions beside >going to a no clean paste?? > >Thanks in advance. > >John > >################################################################ >TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c >################################################################ >To subscribe/unsubscribe, send a message to [log in to unmask] with following >text in the body: >To subscribe: SUBSCRIBE TechNet <your full name> >To unsubscribe: SIGNOFF TechNet >################################################################ >Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section >for additional information. >For technical support contact Hugo Scaramuzza at [log in to unmask] or >847-509-9700 ext.312 >################################################################ > ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################