Jason, Are we talking SOTs here? Wave solder or Reflow? Some PWB designers use the same pad size for SOTs no matter which side of the board they reside on. My experience with wave soldering SOTs so designed is that you will get random skips. The height of the SOT's body, the height at where the leg comes out of the body, and the short length of the leg and a standard reflow pad all contribute to skips. We have found that an extra 0.020" to 0.025" on the length of the wave soldered SOT pad will eliminate solder skips. Gary Camac I'm searching for tricks of the trade for soldering the unbearable 3-legged > transistor. We have the correct orientation on our panel, but seem to still > have problems wave soldering them intermittedly. I would appreciate any help > you can give with soldering them. > > Jason Smith > Process Materials Engineer > Lexmark Electronics > > ################################################################ > TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c > ################################################################ > To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: > To subscribe: SUBSCRIBE TechNet <your full name> > To unsubscribe: SIGNOFF TechNet > ################################################################ > Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. > For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 > ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################