Tim, I was running into almost the same problem(bowing) when trying to replace PBGA 388. Bowing of the corners is caused by excess heat coming from the corners of the nozzle that you're using. Increase the preheat time so that the temp across the component is more stable. Warpage on the PCB might be due to localized heating of the bottom heaters depending on what rework station you're using. Some will heat up the whole PCB strenghtening the heat under the component. Are the vias still tented after removal of solder on the pads? If the solder mask is removed, solder shorts are eminent. Tom Han Ardent Systems On Sat, 31 Oct 1998 07:29:00 -0500 "Stammely, Tim" <[log in to unmask]> writes: >Hello all, > >We are trying to remove and replace two ORCA 432 pin BGA's on a big >14-layer >board. We are getting alot of shorts after the rework(I'm x-ray >inspecting). >At first we tried solder pasting the pads with a mini stencil, but the >amount of bridging we got caused me to try just fluxing the pads and >letting >the solder balls collapse, but we still got a lot of shorts. I am also >noticing a lot of board warpage during the rework heat cycle and it >also >appears that during reflow if I watch the component, the corners of >the BGA >collapse very early and the component almost appears to be bowing. >Most of >the shorts we are getting are in the corners where this last >observation >occurs making me think it is causing the shorts. Any suggestions on >how to >eliminate this problem? > >Thanks, > >Tim Stammely >Manufacturing/Process Engineer >MSI >Manassas, VA > >################################################################ >TechNet E-Mail Forum provided as a free service by IPC using LISTSERV >1.8c >################################################################ >To subscribe/unsubscribe, send a message to [log in to unmask] with >following text in the body: >To subscribe: SUBSCRIBE TechNet <your full name> >To unsubscribe: SIGNOFF TechNet >################################################################ >Please visit IPC's web site (http://www.ipc.org) "On-Line Services" >section for additional information. >For technical support contact Hugo Scaramuzza at [log in to unmask] or >847-509-9700 ext.312 >################################################################ > > ___________________________________________________________________ You don't need to buy Internet access to use free Internet e-mail. Get completely free e-mail from Juno at http://www.juno.com/getjuno.html or call Juno at (800) 654-JUNO [654-5866] ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################