Ken, We use a batch type cleaner here in our facility to clean RMA flux for both SMT and wavesolder CCAs. Machine: Unit Design ABC 2001 Saponifier: Armakleen 2001a Wash cycle (For wave soldered CCAs) : 6 min at 165F % concentration (For wave soldered CCAs): 8 Rinse cycle: (3 times) 1 min at 165F Are you using de ionized water? History here has shown that when source water is not clean enough, that the circuit cards are not clean. Hope that helps. Ron ---------------------- ron rawlyk [log in to unmask] ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################