Hi Angel, For years, the specified solder pot temperature (in military soldering standards and specifications) was 260 +/- 5 C (500 +/- 10 F). As process demands have changed (due in part to increased thermal densities of PCBs and use of heat sensitive parts) in trying to keep the delta temperature from preheat to solder wave contact down below 120 C (one rule of thumb -- will differ per application), the solder pot temperature is dropped to 240 - 260 C (460 - 480 F). There are pros and cons for lowering the solder temperature and I'm sure the metallurgists can better explain this than I, but in laymans terms a higher solder temperature will burn off more flux (less residue) but the solder pot will develop less dross at a lower temperature. Hope this helps. Steve Sauer Sr. Mfg. Engineer Xetron Corporation ---------- From: Angel Luis Ferrandez Berrueco/VLC/EUR/MSL[SMTP:[log in to unmask]] Sent: Tuesday, August 11, 1998 11:03 AM To: [log in to unmask] Subject: [TN] Wave temperature Dear forum colleges. I would thank your help to fix which is the normal temperature for the solder pot in the wave machine. I think that it is between 245 and 250 Celsius, but I have listened 260 Celsius in some occasions. Please could you confirm it? Thank you Angel Ferrandez [log in to unmask] ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################