Charlie, intermetalic formation is a function of time and temp. on the solder dip portion of the HASL process. And, to some lesser extent the porosity of the CU. With acid copper plated on clad "normal" conditions, and with Solder temp at 460f, the range will be from 30 U-inches to as much as 70 to 80 U-inches. Horizontal levellers with good pre heaters produces the shortest dwell times and the thinnest intermetallics. Vertical levellers with no pre heat tend to produce the thicker layers. As far as the free metal above the intermetallic, what your looking for is a "fused" condition of the surface. This occurs in the HASL process at approx. 100 U-inches. The mil spec for years was 300 U-inches, this was borrowed from the venerable T/L plate with oil or IR fusing process. And this is because T/L as plated won't fuse (get shinny) at less than 300 U-inches. The reason you are getting such a large range from your suppliers may be their attempt to account for all coated areas (pads and lands) regardless of shape and size. Try agreeing on specific areas to measure (the smallest are best) this will reduce your range. Hope this helps, if you need more, contact me directly, Mark Simmons ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################