Hi Chris I 'll do the best I can with the information I have. (on goes my flame proof suit again) 1. FR-4 0.062" thick boards absorbs between 0.08 to 0.1%Wt of moisture within a 24 hour period, and 0.2 to 0.23%Wt in 2880 hours (120 days). These measurements were carried out under environmental conditions of 20deg C (max. variation 1degC) and 50%RH (max. variation 3%), using specimen sizes of 40mm x40mm, and FR-4 with a 43% resin content. (Some PCB materials absorb up to about 6 times as much under similar conditions) 2. Assuming you are using standard FR- 4 and not high Tg stuff the Tg would be around 130- 140deg C (TMA). At Tg many properties change abruptly, Young's modulus, shear modulus, specific heat. etc. When heated above the Tg the boards begin to lose mechanical strength due to softening of the resin and often exhibit large discontinuous changes in their out-of- plane CTE. It is these changes which sometimes cause delaminations between the resin and glass fibres in the board, or more commonly between the copper traces and the resin. 3. I think the max. wave soldering temperature in somewhere in the region of 250 deg C. I am not an expert on this but I don't think the actual board temperature exceeds 220deg C. I have been reliably informed that the board temperature exceeds 183 deg C for no more than 90 seconds and is over 140 deg C for about 2.5 minutes. I have in the past measured delamination time for FR-4 at 260 deg C to be between 12 and 15minutes. So although the soldering temperatures exceed the Tg Theoretically it should not be a problem. Factors such as storage conditions prior to wave soldering could be critical. General Below Tg organic substrates are capable of absorbing moisture. although this moisture is static it can still effectively reduce the Tg and consequently the maximum working temperature of the substrate. The rate is highest in the first 24 hrs. (I have not carried out tests over periods less than this) Baking at 105deg c for about 2 hours should get rid of this moisture. The moisture absorption capability is influenced by the degree of cure of the resin, the resin content, and storage conditions of temperature and humidity. Depending on the type of delamination there could also be other causes such as poor interlaminar adhesion or poor Cu adhesion. Ramp rate of solder profile. Additional information can be found in "Circuit world Vol. 12 No 4, 1986 < Blowholing in PTH solder fillets part 3 moisture and the PCB> By M P Seah et al. I hope this helps. F.K.Frimpong. PS. Do you also get delamination during the plating process? Is the delamination characterized by lifting pads, measling under copper layers, glass fiber separation from resin etc. Chris Elliott <[log in to unmask]> on 11/07/98 00:33:05 Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond to Chris Elliott <[log in to unmask]> To: [log in to unmask] cc: (bcc: Frank Frimpong/HQ/CUK/Celestica) Subject: [TN] Delamination Problems We have been having a reoccurring problem with PCB delamination. At first we were thinking that it was a moisture problem. The boards were being stored in our store room open to the ambient air. Once, after two boards in a run delaminated, the assembly house flagged the entire run, and I actually personally took the rest of the boards home to my electric oven to bake. I then re-packed them (warm) in some ammo cans that I have with a desiccant pack in each. None of the baked boards delaminated. We thought that we would solve our problems if we specified for the assembly house to bake the boards and handle them post-bake per IPC-PE-740, (as per a similar discussion here that I found in the archives). All this was with boards from two PCB manufacturers (call them PCHouseA and PCHouseB). Well just recently we got some boards in from a third manufacturer (call them PCHouseC) that we have never used before. (The board is for a product line that we bought from another company so we are still using their resources for purchasing.) We received the boards from them, opened them enough to make a quick visual inspection and immediately sent the boards to our assembly house. Unfortunately, due to communications lags, the board baking didn't happen for that run and we had delamination problems with those boards. Our QC inspector, (thinking that moisture may not be the problem because of the lack of storage time in our stock-room), talked to PCHouseC about this and their thoughts were about wave solder temperature and FR-4 temperature maximums. My questions are: 1. About how long does it take for FR-4 (0.062" thick) boards to absorb moisture? (Any one got (or can point me towards) graphs for this? If so, please use private E-Mail to MIME attach the message.) 2. How would approaching (meeting, or exceeding) the Tg affect the board at the solder wave in such a way as to produce delamination? Is there another critical temperature that I should be aware of here? 3. What wave solder temperature profile is considered 'standard' or 'average'? Many apologizes if any of the above questions are too vague for a concise answer, but I'm learning this stuff as I go... (definite trialby-fire here...) TIA for any help. Pax -- Member: Team AMIGA --} WatchDog Fingerprint: 2C 8A 03 3C D6 D3 32 7F (Chris Elliott) 66 0F 9B 9F 03 77 1D 85 PGP Key ID: A6A79259 <tsb> Experience is directly proportional to the value of equipment destroyed. -- Carolyn Scheppner ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################