The best way to improve surface to hole plating is through the following: 1. Lower metal content and increase acid content to improve conductivity 2. Reduce amps and increase plating time (severely impacts production) 3. Improve solution agitation through the holes 4. Optimize and balance plating films to improve plating distribution from side to side 5. Some single component brightener systems are effective but most people trying to obtain 1:1 on 6:1 aspect ratio boards will end up using multi component brightener system. Call direct if you would like to discuss further -----Original Message----- From: Jason Zhao <[log in to unmask]> To: [log in to unmask] <[log in to unmask]> Date: Wednesday, July 01, 1998 10:12 AM Subject: [TN] Surface to hole ratio of copper plating >Hello, everyone. >I am doing a project to improve our capability and overcome the >overplating issues in copper plating. the vendor suggested us to reduce >the number of anodes to lower the surface to >hole ratio. Would that help? What are the other factors that affect the >surface to hole ratio? we are using electrochemicals PC-667 acid >copper. >Thank you in advance. > >Ja > >################################################################ >TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c >################################################################ >To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: >To subscribe: SUBSCRIBE TechNet <your full name> >To unsubscribe: SIGNOFF TechNet >################################################################ >Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. >For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 >################################################################ > ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################