Hi Jon, If you can keep the stencil opening narrower than the pad width, you will have less bridging and solder balls. You should not make the stencil width too small, however, or you will not get good paste release. (Stencil opening to stencil thickness should be equal to or more than 1.5:1, e.g., .009 opening is smallest usable for a .006 thick stencil.) Another source of solder balls and, sometimes, bridging would be paste on the bottom of your stencil. If you don't have a good seal between the stencil and the pads, the paste will "bloom" on the bottom because of the vacuum being pulled. I believe you have received very good info on the intrusive reflow and the MELF pad design (a "U" shaped pad). Some years ago I made a test board of different shapes, sizes, and spacings of pads for MELFs. You can see real quick, what works best. We wound up using a "U" shaped pad, but I don't recall the dimentions today. Good luck, Charlie Barker Sr. Manufacturing Engineer Input/Output, Inc. Stafford, Texas [log in to unmask] 281-552-3328 Voice Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond to Benedicto Cruz <[log in to unmask]> To: [log in to unmask] cc: (bcc: Charles Barker/US/I-O INC) Subject: [TN] see items stated Hi! I would like to ask for an effective stencil aperture design for fine-pitch ICs. We are encountering some solder bridging on these ICs. Also, there are solder balls present beside these components. Do you have any stencil design guidelines that you could share with us to improve our Screen Print Process? Also, Are you familiar with intrusive reflow? Can anyone share some informaiton about this? We also have a product that uses a MELF SMD resistor. The problem that we are encountering is that this component rolls during solder paste curing. So when it comes out, the component is already misaligned. Do you have any suggestions to control this without using any fixtures? Thanks. Regards. Jon Cruz Electronic Assemblies Inc. Manila, Philippines e-mail: [log in to unmask] Tel #: 823-7317/7593885 Fax #: 7538629 ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################