Possible causes: Based on your description, I suspect that the solder is solidifying at different rates, possibly due to different thermal masses inherent in the circuit layout, a thereby causing the tombstone phenomenon. Are the suspect termination pads attached directly to or totally part of a large copper plane, without thermal reliefs? These pads would solidify more slowly, allowing the termination to lift out of the liquid solder. Perhaps the paste printing process is depositing different paste volumes on the pads? There may be thermal shadowing from adjacent components, but that's probably an unlikely scenario with convection reflow. I've experienced reflow tombstoning similar to yours with a specific type of chip component. The parts are EMI filter-capacitors (also called three-terminal capacitors). They're available in standard package sizes, however, have terminations on all four sides (for example, check the Murata Electronics page <http://www.iijnet.or.jp/murata/products/english/catalog/k01eemi.pdf> using part type NFM40P for a photo and technical specifications). BTW, I'm not affiliated with this company. Are you dealing with this type of device? Completed assemblies are in-circuit tested (shorts & opens, values, orientation, etc.) which is certainly a more consistent process than visual inspection, once equipment and programs are in place. Hope this helps solve the problem. Contact me directly if you want to discuss this further. Ellsworth D. Berkowitz, P.E. Member of Technical Staff Paradyne Corporation phone:813-530-8121 **************************************************************** The opinions expressed herein are solely those of the writer and do not necessarily reflect the views of Paradyne Corporation. **************************************************************** LAMBERT.K.A- wrote: > Hi all, > > We've been working at getting an automated line up and running. We're > making one sided ceramic substrates. The substrates are both low > temperature cofired ceramic and thick film copper. Both have a 63/37 > solder coating on the tracks. The substrates have passed > solderability testing with ease. The pads have been designed > appropriately to minimize tombstoning. Our components are solderable. > We stencil print solder paste onto the substrates. A robot places the > components. Reflow soldering happens in a Nitrogen convection oven. > We are using RMA solder paste (still!) > > Now for the question. Why do we get unsoldered connections? Most are > chip components where one end solders beautifully, the other end is > sitting on a rounded mound of solder. The distribution across the > substrate and from one substrate to the next appears to be random. > > To detect unsoldered connections, we are doing the old brute force > method of having manufacturing personnel looking for them after > reflow. > > What are other folks out there doing to: > 1. Solve the unsoldered connection problem > 2. Detect the unsoldered connections > > Thank you, > > Kathie Lambert > Process Engineer > Northrop Grumman > Baltimore, MD > [log in to unmask] > > ################################################################ > TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c > ################################################################ > To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: > To subscribe: SUBSCRIBE TechNet <your full name> > To unsubscribe: SIGNOFF TechNet > ################################################################ > Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. > For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 > ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ################################################################