Stephan, This topic sounds like it would make an extremely interesting thesis. The cleaning processes you have briefly described would more likely induce oxidation rather than remove it from the spherical surface. When you have a non-uniform sphere geometry after liquidus, it is most likely due to the oxidation concentration on the sphere or pad surface. However, if the spheres are not melted in an inert atmosphere the oxide skin may perpetuate your problems. One of the techniques that I use, and it has been extremely successful, is the use of a plasma cleaning process. There are a number of small reaction chambers on the market. I currently use a March Px1000 system for all development work. There are also hundreds of oxide reducing recipes already in existence however, you may just want to spend some time developing a custom recipe which will best fit your requirements. The following is an example recipe that I have had good results with: Gas 02 Pressure 90 mtorr Power 359 watts Process time 3 min Gas Flow rate 536 sccm Gas Ar Pressure 150 mtorr Power 250 watts Process time 2 min Gas Flow rate 100 sccm Remember that argon etches organic and oxygen cleans organic. With the argon etch atoms are elevated to a higher energy state which with physically displace organic molecules or atoms. Weight loss of the 63/37 may be as high as 0.62E-12 grams per mm2. With the oxygen atom will undergo an oxidation-reduction reaction converting surface organics to water and CO2. There is basically no mass (other than the organic) lost during this process. The trick with your application will be limiting the sputtering effect caused by large molecule inert gasses such as argon, while producing the cleaning effect necessary. William Casey MCMS Research & Development Direct: (208) 898-1042 Fax: (208) 898-2740 [log in to unmask] >---------- >From: Meschter, Stephan J[SMTP:[log in to unmask]] >Sent: Wednesday,May 27,1998 7:39 AM >To: [log in to unmask] >Subject: [TN] BGA Type Solder Sphere Deoxidation > >Hi, >This is my first technet request. I have been reading the net correspondence >with interest over the last month. I think that some of the processing >associated with BGA spheres may be relavent to my problem. > >I am working on my PhD research project which is exploring the melting and >spreading behavior of an initially solid solder sphere placed on copper >substrates held at an elevated temperature in a gaseous formic acid/nitrogen >environment. I have been working mostly with tin and 63Sn/37Pb solder and am >now trying solder spheres with higher lead content. The sphere sizes that I >am using are between 25 and 35 mils in diameter. I found that with the tin >and tin-lead eutectic that some pretreatment of the spheres yield more >consistent melting/spreading behavior. To pretreat my spheres, I place 20-30 >spheres in a 50 ml beaker with an RMA flux at 110-120C for 10 minutes >followed by a series of rinses to get the flux off. Since the flux did not >go up to the solder reflow temperature it is fairly easy to get off. First >the spheres are rinsed in 3 successively cleaner isopropyl alcohol baths at >50-60C (total time 20 minutes) then are put in a final rinse of 30-40C >methanol for 10 minutes followed by blowdrying with nitrogen. > >When I pretreat the high lead content spheres using this method, I see the >spheres darkening as I rinse them...especially when I get to the methanol. >The resulting melting and spreading of these spheres is non-uniform. When I >melt them, it appears that they have an oxide skin on them. I am continuing >to tinker with the rinse process times and solvents to see if I can get a >combination that works. I the mean time, I was wondering if anyone out there >had any ideas. > >I am looking for a sphere pretreatment scheme that will eliminate the oxide >skin and not have any residues on the sphere surface. The process should >not cause preferential etching of the tin or the lead on the sphere surface. > >PS...A while back, as I was developing the my sphere pretreatment process, I >tried using a commercial solder brightener product followed by a DI water >rinse on the 63Sn/37Pb spheres and it didn't really provide the consistency >I had hoped for. I was going to try this again with the high lead content >spheres. > >Thanks in advance for any help that you can offer. > >Steph > >********************************************************* >Stephan Meschter [log in to unmask] >Lockheed Martin Control Systems Phone :(607)770-2332 >600 Main Street, MD R52F FAX :(607)770-2056 >Johnson City, NY 13790-1888 MARCALL: 8 * 255-2332 >********************************************************* > >################################################################ >TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c >################################################################ >To subscribe/unsubscribe, send a message to [log in to unmask] with following >text in the body: >To subscribe: SUBSCRIBE TechNet <your full name> >To unsubscribe: SIGNOFF TechNet >################################################################ >Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional >information. >For technical support contact Hugo Scaramuzza at [log in to unmask] or >847-509-9700 ext.312 >################################################################ > > ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312 ################################################################