Ed, Hydrogen reducing gas atmospheres are pretty common in the hybrid and hermetic packaging industries. I used to work with this sort of stuff with a previous employer. My experience is on hermetic ceramic semiconductor packaging. The seal on these packages was made with 80/20% Au/Sn alloy. The sealing surface on the package was 60 micro inch gold over nickel over Tungsten. During the high temperature die attach process prior to seal there would be Nickel diffusion through the gold and oxidation of the nickel on the surface. The H2 scrub reduced the Nickel oxides back to Nickel and gave a surface solderable without flux in an N2 atmosphere. This worked well provided the delay between scrub and solder seal didn't exceed a couple of days (time for the Nickel to oxidise again). I did quite a bit of work with a University using secondary ion mass spectrometry to get a good process. You need around 78% N2, 12% H2 by volume in the atmosphere Peak temperatures of 30 to 350C work well with times at peak of 1 to 2 minutes. If you are trying to high temperature solder a system that isn't sealed then you can carry out the soldering in the reducing atmosphere without flux. If you are soldering a sealed hermetic package then the soldering should be done in an inert atmosphere after the reducing scrub to keep the moisture content in the sealed package to reasonable levels. The fun part of this process is the safety aspect. You are putting H2 into a belt furnace with open ends. Air is only prevented from getting in by the gas curtains at each end of the belt. You had better make sure that the gas curtains and the furnace atmospheres are balanced. We had an explosion (before my time there) when a design fault on one furnace, where a relay failure allowed H2 and O2 solonoid valves to open simultaneously into a 350C furnace. You need flame offs over the exhaust ports and H2 detectors around the furnace are useful. BTU used to make this sort of equipment. No doubt others do too. Hope this helps Jeremy Drake Celestica Ltd ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ################################################################