The easy answer is to run the commoning connection internally to the card. I realize that this is not always an option. I have experienced a problem similar to what you described on an OSP card. After the external commoning connection was severed a final process step was to microetch clean and apply the OSP. We experienced a galvanic etch at the end of the commoning connection that left a severe gold overhang that would damage connectors. The fix was to better control the microetch clean and make sure the number of passes through OSP was tightly monitored. If none of this makes sense for your particular product, I would simply start by looking at the bevelling tool and how the bit life is controlled for resharpening and changing. Kelly Kovalovsky [log in to unmask] on 03-25-98 10:48:30 PM Please respond to [log in to unmask] To: [log in to unmask] cc: Subject: [TN] Gold -Finger Bevel Issue We are starting to see a small amount of bent connectors from riser cards that exhibit a slight overhang of Gold plating material left after beveling gold finger robber bars off. Does anyone have any ideas of how to design around of illiminate this issue? Thanks ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ################################################################