I too have seen this problem in the past, the voids are caused by outgassing of the material during cure or moisture within the adhesive or in the PCB. If you cure the glue with a fast high temperature profile, the problem is more likely to occur. For example, the adhesive can be cured for 1.5 minutes at 150?C or 2.5 minutes at 125?C. The lower temperature cure is better. Obviously you need to work with the thru-put of your process, but slowing down the cure time worked for us and did not affect thru-put. The voids in the adhesive create a path for the flux and solder (via capillary action), and i have seen shorts under components from one termination to the other of pure solder, or worse yet, solder under the component that did not create a short, but was close enough to the termination that eventually a dendritic growth occured and completed the short. HOWEVER, the main cause of the problem was that the adhesive dot under the component was TOO BIG!! After the component was placed, the adhesive dot covered the entire area under the component and onto the pads. When the component was wave soldered, the pad became liquid, and due to capillary action, solder was sucked into the adhesive voids, thus creating the short. If you make your adhesive dot such that it does not touch the pads or the end terminations then you have eliminated the path for the solder, and thus no more shorts. With this design, even if you have voids in the adhesive and solder is caught in the voids, it does not stretch from pad to pad. Obviously it is best to eliminate the voids altogether. Consider adhesive dot design: With a single dot, make sure that it does not touch the pads or terminations. With a dual dot design: make sure that the dots do not touch the pads or terminations. We also had another problem with dual dots, the gap between the dots also created a pathway for flux or solder. You will find in many books a suggestion to put a dummy trace between the pads. This acts as a dam. The adhesive could be a contributing factor. Hereaus had similiar problems (as was mentioned with Loctite), but they have new formulations(PD944) to help reduce the moisture and outgassing issues. Ed Holton Hella Electronics [log in to unmask] on 02/05/98 09:02:04 PM Please respond to [log in to unmask]; Please respond to [log in to unmask] To: [log in to unmask] cc: (bcc: Ed Holton/Hella North America Inc.) Subject: [TN] Most weird problem: Solder between epoxy & fab or epoxy & comp Dear Technetters, I have seen the most weird problem in my 7 years in PCBA manufacturing environment. Solder is getting between the epoxy and component and/or between fab and epoxy thus shorting it out across terminations of SMT caps. Does any one has seen similar problem? Any resolution? Our regular process is epoxy application thr' stencil, component loading, curing and then hand load & wave. Any help or leads will be highly appreciated. re, ken patel ______________________________________________________ Ken Patel Phone: (408) 490-6804 1708 McCarthy Blvd. Fax: (408) 490-6859 Milpitas, CA 95035 Beeper: (888) 769-1808 ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ################################################################ ################################################################ TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c ################################################################ To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TechNet <your full name> To unsubscribe: SIGNOFF TechNet ################################################################ Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ################################################################