OK, Steve. One thing that I have seen with double treat is that the zinc treatment on the dendrites apparently is thicker than with single treat foil, and when processing through the e'less copper process the inner layer copper is etched back and the zinc "tails" remain. These can give the appearance of a defect. This is only seen with non-catalyzed peroxy-sulfuric or with persulfate etches (I haven't seen too many other types of microetches used); catalyzed peroxy-sulfurics seem to etch away the zinc tails pretty well. I would assume that you know most of the potential reasons for having ICDs (if you want to discuss it, let me know and we'll run through the list). Fred J. >>> Steves <[log in to unmask]> 12/17/97 06:43am >>> Fred J.: I am talking about electroless copper and seperation between the electroless and the innerlayer copper. ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ############################################################## ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ##############################################################