We had similar problems and questions to yours about 2 1/2 years ago. We could not find any facts or users of "Marbles" to reduce dross. I then had stainless steel covers made which float on the solder in configurations to mate up with the solder pot and all items entering and exiting the solder surface. The covers have limited the oxygen to the pot and have minimized dross buildup. The first eight week after installation we did solder contamination testing with no unusual contamination showing. We then dropped back to monthly checks and have not had any problems. Good luck and I hope this helps. Semper Fi Tom >---------- >From: Art G. Pauly[SMTP:[log in to unmask]] >Sent: Wednesday, October 29, 1997 5:13 AM >To: [log in to unmask] >Subject: [TN] WAVE SOLDER DROSS & MARBLES > >I have been having problems with excessive dross build-up in our wave >solder machine. >We are considering adding marbles to the solder pot. I_ve heard >conflicting advice on whether or not this is a good idea. I have heard >that it may keep the dross down, but it may also increase the >contamination levels. Does a dross layer over the marbles protect the >solder from contamination? DOES ANYONE HAVE ANY ADVICE ABOUT DROSS & >MARBLES? > > > -Art Pauly >******************************************* > Art Pauly ([log in to unmask]) > Manufacturing Process Engineer > Kistler Instrument Corporation, USA > Phone: (716)691-5100 Fax: (716)691-5226 > World Wide Web http://www.kistler.com >******************************************* > >############################################################## >TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c >############################################################## >To subscribe/unsubscribe, send a message to [log in to unmask] with following >text in the body: >To subscribe: SUBSCRIBE TECHNET <your full name> >To unsubscribe: SIGNOFF TECHNET >############################################################## >Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional >information. >For the technical support contact Dmitriy Sklyar at [log in to unmask] or >847-509-9700 ext.311 >############################################################## > ############################################################## TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c ############################################################## To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body: To subscribe: SUBSCRIBE TECHNET <your full name> To unsubscribe: SIGNOFF TECHNET ############################################################## Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information. For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311 ##############################################################