Hi Charles, The reasons for problems with the reliability of solderjoibts of TSOPs with Alloy 42 lead/leadframes are threefold: (1) and most important, the Alloy 42 leadframe has a CTE of ~5 ppm/oC whereas FR-4 is ~17+-2ppm/oC, giving you a large global thermal expansion mismatch; (2) solder joints to Alloy 42 are (even under the best of circumstances) weaker than those to copper, and in some cases (perhaps one supplier of Alloy 42 in the Far East (South Korea?)) some Alloy 42 has been found to be virtually non-solderable, a problem HP (see Engelmaier, W., and B. Fuentes, "Alloy 42: A Material to be Avoided for Surface Mount Solder Component Leads and Lead Frames," Proc. Surface Mount International Conf., San Jose, CA, August-September 1994, pp. 644-655; also in Proc. Int. Electronics Packaging Conf. (IEPS), Atlanta, September 1994, pp. 503-516; also in Proc. 19th Ann. Electronics Manufacturing Sem., Naval Air Warfare Center, China Lake, CA, February 1995, pp. 5-20; also in Proc. NEPCON West '95, Anaheim, CA, February-March 1995, pp. 385-395; also in Soldering & Surface Mount Technology, No. 21, October 1995, pp. 20-25) and others have run into; (3) there also exists a local expansion mismatch between Alloy 42 and the solder (CTE~25ppm/oC), which because of the short foot length of the leads is less important. Thus, you need to underfill the TSOPs totally. It is however far better to use TSOPs with copper leadframes. Werner Engelmaier Engelmaier Associates, Inc. Electronic Packaging, Interconnection and Reliability Consulting 23 Gunther Street Mendham, NJ 07945 USA Phone & Fax: 973-543-2747 E-mail: [log in to unmask] *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To subscribe/unsubscribe send a message <to: [log in to unmask]> * * with <subject: subscribe/unsubscribe> and no text in the body. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************